The right steel for a first knife is the one you can heat treat properly with the equipment you have. For most people starting out, that is 1084.
Start with how you will heat treat
A knife steel is only as good as its heat treatment, and steels differ a lot in how much equipment they need. Decide that first, then pick the steel.
- A forge or torch, and a toaster oven kept for the shop. Choose a simple carbon steel that hardens without a long, exact soak: 1084, 1075/1080 or 80CrV2.
- A heat-treat kiln. Everything is open to you, including O1, 1095 done properly, and the stainless steels.
- Sending blades out. A heat-treating service will harden almost any steel for a modest fee per blade. This is the easy way to use stainless without buying a kiln.
Carbon steels
Carbon steels are inexpensive, grind easily and take a keen edge. They rust if left wet and develop a gray patina in use.
| Steel | Good for | What to know |
|---|---|---|
| 1084 | First knives, general use | The most forgiving steel to harden at home. It needs only a short soak at temperature and will harden in warm canola oil. |
| 1075 / 1080 | Larger blades, practice | Behave much like 1084, a little tougher and slightly less wear resistant. |
| 80CrV2 | Hard-use and outdoor knives | Very tough, with better edge holding than 1084. Simple to harden, but ask the seller whether the bar is ready to harden or needs normalizing first. |
| 15N20 | Thin, tough blades; pattern-welded steel | Tough and bright from its nickel. Usually paired with 1084 for damascus. |
| 1095 | Fine-edged slicers, hamon | Needs a controlled soak and a fast quench oil to reach full hardness. Often disappoints when done in a forge by eye. |
| O1 | Fine edges, precision-ground stock | Holds an edge well and is sold ground flat. Needs a soak of 10 minutes or more at temperature, so a kiln is the reliable way. |
| 5160 | Big choppers and swords | Spring steel: very tough, moderate edge holding. |
Stainless steels
Stainless steels resist rust and many hold an edge longer. They harden at much higher temperatures with a timed soak, wrapped in foil or in a controlled atmosphere, and are quenched between aluminum plates. That means a kiln, or sending them out.
| Steel | Good for | What to know |
|---|---|---|
| AEB-L | Kitchen knives, a first stainless | Inexpensive, very tough and fine-grained, so it takes a thin, sharp edge. Edge holding is moderate. |
| 14C28N | Kitchen and everyday knives | Close to AEB-L with a little more corrosion resistance. |
| CPM MagnaCut | Premium all-rounders | Tough, very corrosion resistant and long-wearing. Expensive, and slower to grind and finish. |
| CPM 154 / S35VN | Everyday and hunting knives | Established premium steels with good all-round properties. |
| D2 | Hard-wearing work knives | Not fully stainless. Holds an edge a long time but is harder to sharpen and less tough. |
How thick to buy
Thinner than most beginners expect. A thick blade is stronger, but it cuts worse and takes far longer to grind.
| Knife | Stock thickness |
|---|---|
| Kitchen knives | 1.5 to 2.5 mm (1/16 to 3/32 in) |
| Everyday, hunting and general-purpose knives | 3 to 4 mm (1/8 to 5/32 in) |
| Bushcraft, camp and chopping knives | 4 to 5 mm (5/32 to 3/16 in) |
| Machetes | 2.5 to 3 mm (3/32 to 1/8 in) |
| Swords | 5 to 6 mm (3/16 to 1/4 in) at the guard, thinning toward the point |
| Spearheads | 4 to 6 mm (5/32 to 1/4 in) |
For width, the bar has to cover the tallest point of the profile with a little to spare. BLANKSMITH works this out from your design and names the narrowest standard bar that fits.
Steel for swords and spears
A long blade is picked for toughness before edge holding. It has to flex and come back, and take a bad cut without breaking.
- Good choices: 5160, 8670 and 80CrV2, with 1075 and 1084 close behind. All are oil-hardening, forgiving, and sold in sword lengths.
- Leave for later: 1095, W2 and 26C3 (hard, less tough, and prone to cracking in a long quench), and the stainless and high-alloy steels, which need a kiln as long as the blade.
- Temper softer. Production swords are sold at about 50 to 55 HRC, under a knife. Supplier tables for these steels give about 55 to 56 HRC at 260 °C (500 °F) and 52 to 53 HRC at 315 °C (600 °F), two 2-hour tempers. Softer is not automatically tougher: impact tests on 5160 and 80CrV2 found toughness falling above about 230 °C (450 °F), so test a piece of your own bar.
- Spearheads can be treated like a tough knife: any of the simple carbon steels above, hardened on the blade only, tempered at the soft end of the range or a little under it, with the socket or tang left soft.
For a sword or a spear, see making a sword or a spear.
Typical heat-treat numbers
These ranges cover the recipes published by the sources listed at the end of this guide, which do not all agree. The data sheet from your own steel supplier takes priority, because the right numbers depend on the exact chemistry and the condition the bar is sold in.
| Steel | Harden at | Soak | Quench | Temper (2 × 2 hours) |
|---|---|---|---|---|
| 1084 | 790 to 815 °C (1450 to 1500 °F) | 5 to 15 minutes in a kiln | Fast oil such as Parks 50, or warm canola | 205 °C (400 °F), about 60 to 61 HRC |
| 80CrV2 | 795 to 830 °C (1465 to 1525 °F) | 5 to 20 minutes, longer for thicker stock | Oil | 205 °C (400 °F), about 60 to 61 HRC |
| 1095 | 800 °C (1475 °F) | 5 to 10 minutes | Fast oil such as Parks 50 | 205 °C (400 °F), about 60 to 62 HRC |
| O1 | 795 to 805 °C (1465 to 1480 °F) | 10 to 30 minutes | Medium-speed oil | 205 °C (400 °F), about 60 to 61 HRC |
| AEB-L | 1065 to 1080 °C (1950 to 1975 °F) | 15 minutes, in foil | Aluminum plates, then a cold treatment if you can | 175 °C (350 °F), about 61 to 62 HRC |
Without a kiln, a magnet is the usual guide for the simple carbon steels: the steel stops attracting a magnet a little below its hardening temperature, so heat it evenly to just past that point and quench. Temper as soon as the blade is cool enough to hold; an untempered blade is brittle enough to crack if dropped.
Where to buy
Buy from a knife-steel supplier, not a general metals yard: the bar arrives annealed, in knife-friendly sizes, with a known chemistry.
- New Jersey Steel Baron: knife steel bar stock.
- Pops Knife Supply: steel, handle material and belts.
- Alpha Knife Supply: specialty steels and handle materials.
BLANKSMITH is not paid for these links today; some may earn a commission in the future. See the disclosure.
Pick the steel in your design
Choose a steel in BLANKSMITH and it gives you a heat-treat card for it, the bar size to order and the cost per knife.
Sources
- Knife Steel Nerds: How to heat treat 80CrV2
- Knife Steel Nerds: How to heat treat knife steel in a forge
- Pops Knife Supply: Heat treating and tempering information
Heat-treat figures checked against these sources on 19 November 2026.